Surface Finishing for Robot Structural Parts: A Dimension Decision, Not a Cosmetic One

Nov 20, 2026

Leave a message

Surface Finishing for Robot Structural Parts: A Dimension Decision, Not a Cosmetic One

A robot's bracket does not need to look good. It needs to survive coolant, hold a bearing fit for five years, and not corrode against the steel screw next to it. Every one of those is a coating specification - and every coating changes the size.

 

Four jobs, not one

"Surface treatment" on a robot drawing is usually a single line at the bottom. In practice it is four different requirements that often conflict.

Requirement

What it is really asking

Typical answer

Wear resistance

The face rubs, slides or is assembled repeatedly

Hard anodising, hard chrome, electroless nickel

Corrosion resistance

Coolant, washdown, humidity, outdoor air

Anodising, chem film, plating, painting

Appearance

The part is seen by the customer

Powder coat, anodising in colour

Functional interface

Conductive, insulating, low outgassing, cleanable, ESD

Chem film, conductive anodising, passivation, electropolish

A joint housing can need three of these at once: hard anodised on the bearing bore, chem film on the mating faces, powder coat on the outside. That is three processes, three masking operations, and three chances to lose a dimension.

img-mworzjxe-b9bda0d0

The thing everyone forgets: coatings have thickness

This is the single most useful fact in the article.

An anodic film does not sit on top of the aluminium - roughly half grows inward and half outward. So a 20 µm anodic film changes the external size by about 10 µm, and it changes a bore in the opposite direction: the hole gets smaller by about 10 µm and the surface gets harder.

Plating is different. Electroless nickel and hard chrome build entirely outward, so a 25 µm nickel layer adds 25 µm to every surface it touches - including the inside of a bore, which closes by 50 µm on diameter.

Process

Typical thickness

Effect on size

Notes

Chem film (conversion coating)

0.3–3 µm

Negligible

Best choice when dimensions are tight

Sulphuric anodising

10–25 µm

~half in, half out

Standard corrosion finish for aluminium

Hard anodising (Type III)

25–50 µm, up to 100+

~half in, half out, more on radii

Wear surface; brittle, cannot be bent after

Electroless nickel

5–25 µm

Fully outward

Uniform on complex shapes; good corrosion

Hard chrome

20–50 µm+

Fully outward

Wear and rebuild of worn shafts

Zinc or zinc-nickel plating

5–15 µm

Fully outward

Steel fasteners and brackets

Passivation

Sub-micron

None

Stainless only; removes free iron

Electropolishing

Removes 10–30 µm

Size decreases

Medical and cleanroom surfaces

Bead blasting

Removes 5–20 µm

Size decreases; edges round

Preparation, not a finish on its own

Two consequences follow immediately:

1. State the finish before the drawing is released, not after. A ±0.02 mm bore tolerance and a 25 µm nickel layer cannot both be honoured unless the bore is specified undersize or masked.

2. Mask the fits, or machine after coating. For hard anodising, machining after coating is not an option - you cut through the hard layer and lose the wear surface. So the bore must be masked, or grown by the right amount.

img-mworzxo5-1def785c

Matching the process to the part

Aluminium housings and brackets. Sulphuric anodising for general corrosion protection, hard anodising where a face rubs or a bore takes a repeatedly inserted pin. Chem film (chromate-free where required) when dimensions matter or when the part must conduct. Never anodise a part that will be a ground path - the film is an insulator, which is why conductive anodising exists as a separate, more expensive option.

Steel shafts, pins and inserts. Hard chrome for wear and for rebuilding a worn diameter. Electroless nickel where the geometry is complex and the coating must be uniform. Zinc-nickel for fasteners that see salt spray.

Stainless parts. Passivation to remove free iron from machining, and electropolishing where cleanability or a low particle count matters. Neither changes the size meaningfully, which makes stainless attractive for tight assemblies.

Magnesium. Always coated, always isolated. A bare magnesium part in a robot will corrode visibly within weeks in a humid plant. Chem film plus powder coat, and isolation from steel fasteners.

Titanium. Anodising for wear and for colour coding, passivation for cleanliness. Titanium against aluminium is a galvanic couple; treat both.

img-mwos0iuw-2ba990a0

Galvanic corrosion is a design problem, not a coating problem

A robot is a stack of dissimilar metals: aluminium housing, steel screw, stainless dowel, titanium insert. Add coolant and time, and the least noble metal becomes the anode.

The coating helps, but it is not sufficient on its own. What actually works:

Break the electrical path with an insulating washer or a coated face.

Keep the joint dry by design - a drain path beats a seal that traps water.

Choose the couple deliberately: anodised aluminium against stainless is far less aggressive than bare aluminium against cadmium-plated steel.

Never rely on paint at a bolted joint. The bolt cuts through it on assembly, and that is exactly where corrosion starts.

img-mwos0l6z-e561f92d

Finishing for the application, not for the catalogue

Cleanroom and semiconductor robots. Low particle shedding and cleanability. Electropolished stainless, hard anodised aluminium with a sealed film, and no dry-film lubricant that can migrate.

Medical and laboratory. Repeated wipe-down or autoclave. Passivated stainless, anodised aluminium, and coatings that survive the cleaning agent - check the chemistry, not just the temperature.

Food handling. Washdown with caustic and acid. Stainless with passivation, or a coating system approved for food contact. Anodised aluminium is generally acceptable for non-contact structure, not for the product contact surface.

Outdoor and mobile robots. UV and salt. Powder coat over chem film, with the film doing the corrosion work and the powder doing the UV work - a powder coat alone on aluminium will fail at a scratch, because there is nothing under it to stop the corrosion spreading sideways.

Collaborative robots. The outer surface is touched all day: wear, cleaning agents, and appearance. Powder coat is the practical answer; hard anodising is better where the surface is also a wear face.

img-mwos0p5s-bbdab802

Hydrogen embrittlement: the one that breaks parts silently

Any high-strength steel - roughly above 1,000 MPa, or harder than about 32 HRC - that is electroplated absorbs hydrogen. It does not fail at assembly. It fails weeks later, under load, with no warning.

The requirement is a bake: typically 190–220 °C for several hours, started within a defined window after plating (often within one to four hours), and before any grinding or bending. Acid pickling before plating is part of the same risk.

If a supplier plates a hardened steel pin and cannot state the bake schedule, treat the part as unverified. This is not a detail that can be inspected afterwards.

img-mwos0mxd-7c163cda

Inspection: what to measure, and with what

What

Method

When it matters

Coating thickness

Eddy current (anodising on Al), magnetic (plating on steel), X-ray fluorescence

Every coated part; check bores too

Adhesion

Cross-hatch, or pull-off

Painted and powder-coated parts

Corrosion resistance

Neutral salt spray to ISO 9227

Specification-driven; hours, not "passes"

Surface hardness

Microhardness (HV) on a coupon or witness piece

Hard anodising, hard chrome

Appearance

Colour and gloss against an agreed sample, ΔE where specified

Visible parts, colour-coded parts

Masking

Visual and dimensional check on the masked features

Any part with fits

Hydrogen bake

Process record, not inspection

Hardened steel, electroplated

The salt-spray number deserves a warning: 500 hours of NSS is not a lifetime prediction, and two suppliers can both "pass 500 h" with very different corrosion behaviour in service. Ask what the failure criterion was.

Five mistakes that cost real money

1. Specifying the finish after the drawing is approved. The tolerance was already set for bare metal.

2. Anodising a threaded hole. The thread grows, the screw binds, and the film is brittle - it cracks off under load. Mask threads, or chase them after coating with a tap that is approved for the purpose.

3. Forgetting blind holes. Acid and rinse water stay in a blind hole and leak out later, staining the part and corroding the mating surface. Specify the drain and verify it.

4. Mixing finishes on one datum face. Half chem film, half anodised, on the same mounting face means the part sits at an angle.

5. Powder coating over a sharp edge. The film pulls back at the edge, leaving the thinnest coating exactly where corrosion starts. Radius the edges, or accept a primer.

What to write on the drawing

A finish callout that a shop can actually execute contains five things:

1. The process and the standard - for example hard anodising to MIL-A-8625 Type III, Class 1.

2. The thickness range, not a single number.

3. The colour or appearance requirement, if any.

4. Which areas must be masked, shown on the drawing rather than described in a note.

5. The corrosion test and its acceptance criterion, if the part is specified by performance.

Add the material temper, because anodising response depends on alloy and temper - 6061-T6 and 7075-T6 do not produce the same film, and 7075 darkens noticeably.

 

About the manufacturer

Shenzhen Strongd Model Technology Co., Ltd. machines and finishes robot structural parts - joint housings, mounts, flanges and links - with robotics accounting for 48% of revenue. The 40,000 m² plant in Shenzhen runs 85 CNC machining centres, 18 of them five-axis, with anodising, passivation, plating, electroless nickel and powder coating available in-house. Inspection uses Hexagon CMM under ISO 9001:2015 and IATF 16949:2016. Prototypes ship in 3–7 days; quotations are returned within 8 working hours.

Website: https://www.strongdcnc.com/

Send Inquiry